Fiilo Flux-Cored ah EC410NiMo

Sharaxaad Gaaban:

EC410NiMo waa silig bir ah oo aan miridh lahayn oo martensitic ah oo leh qaab kiimiko ah oo ka kooban 11.0 – 12.5% ​​Cr, 4.0 – 5.0% Ni, iyo 0.40 – 0.70% Mo.

Faahfaahinta Badeecada

Calaamadaha Alaabta

Heerka u dhigma

GB/T 17853-2018 TS410NiMo-FC11

AWS A5.22M-2012 E410NiMoT1-1

Maaddada u dhiganta: 13Cr-4Ni (EN1.4313/UNS S41500)

Sharaxaad

EC410NiMo waa silig bir ah oo aan miridh lahayn oo martensitic ah oo leh qaab kiimiko ah oo ka kooban 11.0 – 12.5% ​​Cr, 4.0 – 5.0% Ni, iyo 0.40 – 0.70% Mo. Waxay ku habboon tahay dhammaan booskaAlxanka qaansada ee qulqulka-core(FCAW) oo leh qaanso deggan, kala firdhis yar, iyo si fiican u goyn kara slag. Birta la dhigay waxay leedahay iska caabin wanaagsan oo xirasho, iska caabin dildilaac, iyo sifooyin farsamo. Kuleyl hore oo heerkul ah 150 - 260℃ ayaa lagu talinayaa, iyo daaweynta kulaylka ka dib alxanka (PWHT) oo ah 590 ~ 620℃ muddo 1 saac ah (oo ay ku xigto qaboojinta hawada, AC) ayaa loo baahan yahay ka dib alxanka.

Codsiga

Ku habboon alxanka ASTM CA6NM birta la shubay iyo birta taxanaha ah ee 13%Cr – 4%Ni. Waxaa loo isticmaalaa dayactirka adag ee biraha wiishka, duubayaasha daabacaadda, ulaha birta, qaybaha korontada biyaha ee cavitation-ka xiran, iyo qaybaha dhismaha ee u baahan daxalka iyo iska caabbinta xirashada.

Halabuurka Kiimikada ee Birta Alxanka (%)

Walax C Cr Ni Mo Mn Si P S Cu
Shuruudaha ≤0.06 11.0-12.5 4.0-5.0 0.40-0.70 ≤1.00 ≤1.00 ≤0.040 ≤0.030 ≤0.75
Natiijada Imtixaanka 0.02 12.3 4.65 0.54 0.59 0.33 0.023 0.01 0.01

Sifooyinka Farsamada ee Birta La Dhigay

Magaca Imtixaanka Xoogga Laabista (MPa) Kordhinta% Raajo X-Ray Tijaabada Saamaynta(+20℃)J Adkaanta HB Haydarojiin Kala-baxa (ml/100g)
Shuruudaha ≥760 ≥15 Darajada 1aad - - ≤5
Natiijada Imtixaanka 845 19 Darajada 1aad 60-90 250-310 ≤5

 

Halbeegga Alxanka ee lagu taliyay

Isha Korontada: DC Reverse (DC-)

Dhexroorka Silig iyo Hadda:

Hadda lagu taliyay:

Dhexroorka Usha (mm) 3.2 4.0 5.0
Hadda Alxanka (A) 80-120 120-160 150-190

Ogeysiis

1. Ku kari elektaroolka 300℃ saacad ka hor intaadan isticmaalin si aad uga saarto qoyaanka.

2. Nadiifi miridhku, saliidda, iyo qoyaanka dusha sare ee birta; isticmaal hawlgal qaanso gaaban oo loogu talagalay kuul cidhiidhi ah oo alxanka ah.

3. PWHT waa in la sameeyaa isla markiiba ka dib alxanka si looga fogaado xoqidda.

 

 


  • Kii hore:
  • Xiga: