Nickel Alloy Welding Wire ERNiCr-3 Mig Welding Wire

Sharaxaad Gaaban:

ERNiCr-3 waxaa loo isticmaalaa alxanka ee Alloys 600, 601, 690, 800 iyo 800HT iwm.


Faahfaahinta Alaabta

Tags Product

Alloy NickelXargaha alxankaERNiCr-3

Heerarka
TS EN ISO 18274 - Ni 6082 - NiCr20Mn3Nb
AWS A5.14 - ER NiCr-3

 

Tilmaamaha iyo Codsiyada

Alloy 82 waxaa loo isticmaalaa alxanka ee Alloys 600, 601, 690, 800 iyo 800HT iwm.

Biraha alxanka lagu shubay waxay leedahay xoog sare iyo iska caabin daxalka wanaagsan, oo ay ku jiraan iska caabinta oksaydhka iyo xoogga dillaaca gurguurta ee heerkul sare.

Ku habboon codsiyada alxanka ee aan la midka ahayn ee u dhexeeya noocyo kala duwannikkelAlloys, biraha aan kala go'a lahayn, birta kaarboonka oo ay ku jiraan dusha sare.

Ku habboon codsiyada u dhexeeya cryogenic ilaa heerkul sarreeya taasoo ka dhigaysa daawaynta mid ka mid ah kuwa ugu badan ee loo isticmaalonikkelqoyska.

Nabarka lakabka saxda ah ee sifooyinka quudinta siliga sare.

Caadi ahaan loo isticmaalo soosaarka tamarta iyo warshadaha petrochemical iwm.

Qalabka Saldhigga Caadiga ah

Alloy 600, Alloy 601, Alloy 690, Alloy 800, Alloy 330*
* Tusaale, ma aha liis dhamaystiran

 

Halabuurka Kiimikada %

C%

Mn%

Fe%

P%

S%

Si%

max

2.50

max

max

max

max

0.05

3.50

3.00

0.030

0.015

0.50

Cu%

Ni%

Co%

Ti%

Cr%

Nb+Ta%

max

67.00

max

max

18.00

2.00

0.50

min

1.00

0.75

22.00

3.00

 

Xoogga Jilicsan ≥600 MPa
Xoogga Wax-soo-saarka ≥360 MPa
Dheeraynta ≥30 MPa
Xoogga Saamaynta ≥100 MPa

Guryaha makaanikada waa qiyaas waxayna ku kala duwanaan karaan kuleylka, gaaska gaashaanka, cabbirada alxanka iyo arrimo kale.

 

Gaasaska gaashaanka

TS EN ISO 14175 - I1, I3

 

Goobaha alxanka

TS EN ISO 6947 - PA, PB, PC, PD, PE, PF

 

Xogta Baakadaha

Dhexroorka

Miisaanka

Spool

Pallet Qty

1.00 mm

1.20 mm

15 Kg

15 Kg

BS300

BS300

72

72