Heerka jawaab celinta
-NB/T 47018.3-2017 S410NiMo
-GB/T 29713-2013 S410NiMo
-AWS A5.9M-2022 ER410NiMo
-ASME SFA-5.9M-2023 ER410NiMo
-YB/T 5092-2016 H05Cr12Ni4Mo
Maaddada u dhiganta: 1.4317 GX4CrNi13-4,1.4313 X3CrNiMo13-4,1.4407 GX5CrNiMo13-4,1.4414 GX4CrNiMo13-4,ACI Gr. CA6NM
Sharaxaad
ER410NiMo waa silig bir ah oo aan miridh lahayn oo leh qaab kiimiko ah oo leh 11.0 – 12.5% Cr, 4.0 – 5.0% Ni, iyo 0.40 – 0.70% Mo. Waxay ku habboon tahay alxanka gaaska lagu ilaaliyo (sida TIG/MIG) dhammaan boosaska. Inta lagu jiro alxanka, qaansada waa mid deggan, birta la dhigayna waxay muujisaa iska caabin cavitation oo aad u fiican, iska caabinta xirashada ciidda,
iyo sifooyinka farsamada. Guud ahaan looma baahna in la kululeeyo kahor alxanka; daaweynta kulaylka ka dib alxanka (PWHT) oo ah 580 ~ 620℃ muddo 2 saacadood ah (oo ay ku xigto qaboojinta hawada, AC) ayaa lagu talinayaa sida waafaqsan shuruudaha codsiga. Birta la dhigay waa la farsamayn karaa waxayna ku habboon tahay qalabka cadaadiska.
Codsiga
Waxaa loogu talagalay alxanka ASTM CA6NM birta la shubay, birta aan la karin ee 410/410S/405, iyo birta taxanaha ah ee 13%Cr – 4%Ni. Codsiyada caadiga ah waxaa ka mid ah qalabka cadaadiska (oo u hoggaansan heerarka xididdada cadaadiska), daabyada marawaxadaha, waalka, dhuumaha cadaadiska sare leh, iyo qaybaha dhismaha ee u baahan daxalka iyo iska caabbinta xirashada.
Halabuurka Kiimikada ee Birta Alxanka (%)
| Walax | C | Cr | Ni | Mo | Mn | Si | P | S | Cu |
| Shuruudaha | ≤0.06 | 11.0-12.5 | 4.0-5.0 | 0.40-0.70 | ≤1.00 | ≤0.60 | ≤0.050 | ≤0.020 | ≤0.75 |
| Natiijada Imtixaanka | 0.011 | 12.21 | 4.70 | 0.54 | 0.58 | 0.47 | 0.016 | 0.008 | 0.01 |
Sifooyinka Farsamada ee Birta La Dhigay
| Magaca Imtixaanka | Xoogga Laabista (MPa) | Kordhinta% | Raajo X-Ray | Tijaabada Saamaynta(+20℃)J | Adkaanta HB |
| Shuruudaha | ≥760 | ≥15 | Darajada 1aad | - | - |
| Natiijada Imtixaanka | 830 | 18 | Darajada 1aad | 65 | 250-310 |
Halbeegga Alxanka ee lagu taliyay
Gaaska Difaaca: Argon (Ar) ama Ar+1-2% O2 (alxanka TIG/MIG, u hagaaji iyadoo loo eegayo hababka gaarka ah).
Ogeysiis
1. Hubi in dusha sare ee siligga uu nadiif yahay oo uusan lahayn saliid, miridhku, ama qoyaan ka hor inta aan la isticmaalin si looga fogaado saameynta tayada alxanka.
2. Ilaali daahirnimada gaaska iyo heerka socodka saxda ah si looga hortago daloolada iyo dildilaaca ay keento haydarojiin.